Dear Daniel,
I assume that these components are moisture-sensitive. If they have absorbed too much moisture prior to reflow you might be experiencing popcorning. This typically shows up as a bulge over the surface of the die, in the center of the package. The bulge can be on the top side or bottom side of the component. If it is on the bottom and the component has a fairly low standoff (distance between body of component and bottom of leads) this can be enough to lift some leads off the pads on the PCB. In most cases these deformations are on the bottom side and thus impossible to detect with a normal lead standoff.
In any case, to verify if moisture is causing this problem, simply bake your components prior to assembly, at 125C for 48 hours or less, based on moisture sensitivity level and body thickness (ref. joint IPC/JEDEC standard J-STD-033, available for free at http://www.jedec.org).
Please note that if you are experiencing popcorning you should be concerned about other assemblies that can contain damaged component. The parts that do exhibit popcorning represent the most severe case of internal delamination and they may still pass electrical test. However, partial cracks and delaminations that cannot be detected may also cause potential field failures.
If the problem is not related to moisture then it is most likely a design issue with the component and you should consult your supplier.
Good luck !